Casting Defect - Surface roughness

2023-05-12
Characteristic features
The casting surface exhibits a level of roughness corresponding to the size of the sand grains.

Incidence of the defect
The defect primarily occurs near the gate and in very hot areas, and is frequently to be regarded as an early stage of penetration.
The defect is also found at positions where mould compaction is poor.

Possible causes


Clay-bonded sand

? Sand grains too coarse
? Too little lustrous carbon producer in the moulding sand
? Too few fines in the sand.


Moulding plant

? Too little compaction
? Too much adhesion of sand grains to the pattern
? Too little bonding of the sand grains in the mould surface


Gating and pouring practice

? Pouring temperature too high
? Metallostatic pressure too high

Remedies


Clay-bonded sand

? Use fine-grain sand. If necessary, refine core sand so as to adjust the fineness of the recirculating sand
? Increase production of lustrous carbon in the moulding sand. Adjust “active carbon content” to 0.35 % – 0.45 %
? Use carbon carrier that produces more lustrous carbon.
? Increase fines content. Increase coke formation in moulding sand if necessary increase return of dust in order to increase fines content.


Moulding plant

? Improve mould compaction. Increase compacting pressure. Improve sand distribution to achieve more uniform mould compaction.
? Reduce adhesion of sand grains to the pattern. Use a release agent or use it more frequently. Sufficiently heat pattern.
? Improve bonding of sand grains at the mould surface. Avoid rapid drying-out of the surface by means of better development.


Gating and pouring practice

? Reduce pouring temperature

? Improve gates. Avoid local overheating


ABOUT  KEVA
Keva Casting is a professional casting company that focuses on Construction, Machinery, Automobile, Hardware, Pipeline and many other industries.
We provide top quality products with the best service based on our complete production chain including our own mold design, advanced production techniques, and full management of the supply chain. Keva Casting has two factories located in Zhucheng, China's Shandong province.
We use "shell molding", which is a new technique that has been developed in recent years.This new technique has simplified production procedures and reduced air pollution compared with traditional sand casting and investment casting. Shell making and core making are faster to ensure production in enormous quantities. The dimensions and surface finishing are satisfactory for all kinds of industrial requirements. Besides supplying our own formwork & scaffolding systems, our casting products also supply OEM services in various industries.

主站蜘蛛池模板: 美日韩一级大黄片| 美国一级特级大片| 欧美精品久久一级片| 黄片视频大全免费版| 一级做a爰片久久毛片A片477| 国产黄色一级二级片| 一级A片免费看久久夜夜夜| 黄色三级毛片AVaaaa| 欧美黄色网一级片| 一级黄色录像18岁| 一级免费成人黄色片| 国产黄黄色农村女人一级毛片| 黄色一级视频看看吗| 黄片大全免费在线观看禁止| 日韩短视频在线观看| 一区和二区特级黄色片| 中国欧美一级黄色片| 成人免费看一级A片梅花三| 黄色一级片视频免费观看| 国产精品精品一级黄片| 亚洲se三区四区| 一级黄色高清视频免费的| 亚洲无码在线观看卡三| 国产A级毛片精品| 美国一级黄色欧美专区| 黄色A级免费电影免费| 亚洲AV无久久精品一区二区| 欧美a级黄片在线播放| 欧美一级久久小说网| 国产香蕉超级黄片| 国产黄色视频高清| 日韩A级片电影在线播放| 看国产一级黄色录像| 在线免费观看黄片大全| 国产一区无码在线视频| 人与善交一级毛片A片视频下载| 免费在线观看a级片| 黄色一级黄色毛片| 国产一区二区视频在线看| 在线视频免费日韩产| 7日韩一级电影在线观看|